断裂伸长率 | 855% | 拉伸强度 | 36MPa | 密度 | 0.924g/cm3 |
熔体流动速率 | 1g/10min | 用途级别 | 薄膜级 | 规格级别 | 薄膜 |
缺口冲击强度 | 9 |
|
产品简述
断裂伸长率 | 855% | 拉伸强度 | 36MPa | 密度 | 0.924g/cm3 |
熔体流动速率 | 1g/10min | 用途级别 | 薄膜级 | 规格级别 | 薄膜 |
缺口冲击强度 | 9 |
详细数据
订购指南
性能项目 | 试验条件[状态] | 测试方法 | 测试数据 | 数据单位 | ||
基本性能 | 薄膜厚度 | ASTM D-746 | 50 | μm | ||
熔融指数 | ASTM D-1238 | 1.0 | g/10min | |||
密度 | ASTM D-1505 | 0.924 | g/cm3 | |||
机械性能 | 撕裂强度 | MD | ASTM D-1992 | 4 | g/μm | |
TD | ASTM D-1992 | 11 | g/μm | |||
拉伸强度 | (断裂点)MD | ASTM D-882 | 453 | kg/cm2 | ||
(断裂点)TD | ASTM D-882 | 370 | kg/cm2 | |||
拉伸强度 | (屈服点)MD | ASTM D-882 | 135 | kg/cm2 | ||
(屈服点)TD | ASTM D-882 | 120 | kg/cm2 | |||
抗冲击强度 | Spencer | ASTM D-3420 | 9 | kg.cm | ||
伸长率 | MD | ASTM D-882 | 765 | % | ||
TD | ASTM D-882 | 855 | % | |||
热性能 | 脆化温度 | ASTM D-746 | <-70 | ℃ | ||
维卡软化点 | ASTM D-1525 | 102 | ℃ | |||
其它性能 | 添加剂 | SK Method | A/B | |||
雾度 | ASTM D-1003 | 22 | % |